Tantalum tube manufacturing process

Back From: Date: 2020-12-04

Tantalum tube manufacturing process

Tantalum cannot be processed in the usual way that ordinary metals are processed. Generally, the initial process is forging and heat treatment, using hammering and stamping two ways to make plate blank or round small and medium-sized blank.

Bloom

Tantalum cannot be processed in the usual way that ordinary metals are processed. Generally, the initial process is forging and heat treatment, using hammering and stamping two ways to make plate blank or round small and medium-sized blank. Unlike ordinary metals, tantalum cannot be hot worked. If the recrystallization temperature of tantalum is over 1000 ~ C, excessive oxidation will occur even if the general protective coating is made. What's more serious is that if tantalum is exposed to such high temperature, not only excessive oxidation will occur on the surface of tantalum, but oxygen can also invade between atoms in the matrix, making tantalum brittle. Not only oxygen, but also nitrogen, carbon and hydrogen can make tantalum brittle. Due to the above reasons, tantalum is generally not hot worked. When hot working is necessary, protective coating or inert gas atmosphere shall be applied.

heat treatment

Due to the active reaction of tantalum with oxygen, it is necessary to avoid heat treatment in the atmosphere even in the presence of a little air. Therefore, almost all annealing is carried out in a high vacuum, and the furnace must be air tight. Generally, the heat treatment temperature of tantalum is 950 ~ 1300 ℃, and there is no phase transformation between tantalum and tantalum alloy in this temperature range. The heat treatment is only used for annealing, so the heating temperature and cooling rate are not important. In order to produce complete recrystallization, the heat treatment time is better.

Tantalum produced commercially is of high purity. The grains become very large by annealing. The size of crystal particles is determined by cold working, purity, temperature and process steps. Therefore, temperature control and process control are important means to determine the crystal size.

Tantalum, unlike many other metals, must be very clean before heat treatment. If it is not cleaned very clean, the surface contamination caused by hydrogen, oxygen, nitrogen and carbon will occur and become brittle (hardening) structure. Because hydrogen, oxygen, nitrogen and carbon are very active intrusive elements in the temperature range of tantalum annealing, once polluted by these elements, they can be removed except remelting.

Service Hotline

0086-0917-3243231
WeChat
TEL:

0086-0917-3243231

亚洲成av人片在线观看天堂无码| 麻花豆传媒剧国产免费| 特级毛片在线大全免费播放| 亚洲国产精品久久久久婷婷老年| 国产AV无码专区亚洲AV麻豆丫| 日本熟妇中文字幕三级| 亚洲国产精品综合久久网络| 日本乱偷人妻中文字幕在线| 国产av无码专区亚洲a∨毛片| 国产偷窥真人视频在线观看| 国产成人精品2021| 日韩精品免费一线在线观看| 午夜大胆裸体A级人体片| 免费无码成人AV片在线| 亚洲精品无码伊人久久| 中文字幕人成乱码中文乱码| 亚洲精品高清国产一久久| 风流老熟女一区二区三区| 国产真实夫妇交换视频| 97PORM国内自拍视频| 一本一道人人妻人人妻αv| 激情 自拍 另类 亚洲| 国产办公室秘书无码精品99| 亚洲av无码一区二区三区dv| 福利免费观看体检区| 精品无码AV无码免费专区| 亚洲 欧美 小说| 午夜男女无遮掩免费视频| 婷婷成人丁香五月综合激情| 八戒理论片午影院无码爱恋| 熟妇人妻不卡中文字幕| 欧美亚洲日韩不卡在线在线观看| 中文精品一区二区三区四区| 欧美成人免费做真爱| 国产精品福利2020久久| 精品国产免费第一区二区三区| 欧美黑人巨大videos精品| 好男人社区WWW在线观看| 一个人看的www视频免费观看| 亚洲中文久久精品无码WW16| 亚洲AV无码男人的天堂|